Sintered SmCoMagnetSifat Fisik | |||||||||
Bahan | sasmita | Remanence | Pdt. Temp.- Coeff. Saka Br | Kekuwatan Paksa | Kekuwatan Koersif Intrinsik | Pdt. Temp.-Coeff. saka Hcj | Maks. Produk Energi | Maks. Suhu operasi | Kapadhetan |
Br (KG) | Hcb (Panjenengan) | Hcj (Panjenengan) | (BH) maks. (MGOe) | g/cm³ | |||||
SmCo5 | XG16 | 8.1-8.5 | -0,050 | 7.8-8.3 | 15-23 | -0.30 | 14-16 | 250 ℃ | 8.3 |
XG18 | 8.5-9.0 | -0,050 | 8.3-8.8 | 15-23 | -0.30 | 16-18 | 250 ℃ | 8.3 | |
XG20 | 9.0-9.4 | -0,050 | 8.5-9.1 | 15-23 | -0.30 | 19-21 | 250 ℃ | 8.3 | |
XG22 | 9.2-9.6 | -0,050 | 8.9-9.4 | 15-23 | -0.30 | 20-22 | 250 ℃ | 8.3 | |
XG24 | 9.6-10.0 | -0,050 | 9.2-9.7 | 15-23 | -0.30 | 22-24 | 250 ℃ | 8.3 | |
XG16S | 7.9-8.4 | -0,050 | 7.7-8.3 | ≥23 | -0.28 | 15-17 | 250 ℃ | 8.3 | |
XG18S | 8.4-8.9 | -0,050 | 8.1-8.7 | ≥23 | -0.28 | 17-19 | 250 ℃ | 8.3 | |
XG20S | 8.9-9.3 | -0,050 | 8.6-9.2 | ≥23 | -0.28 | 19-21 | 250 ℃ | 8.3 | |
XG22S | 9.2-9.6 | -0,050 | 8.9-9.5 | ≥23 | -0.28 | 21-23 | 250 ℃ | 8.3 | |
XG24S | 9.6-10.0 | -0,050 | 9.3-9.9 | ≥23 | -0.28 | 23-25 | 250 ℃ | 8.3 | |
Sm2Co17 | XG24H | 9.5-10.2 | -0,025 | 8.7-9.6 | ≥25 | -0.20 | 22-24 | 350 ℃ | 8.3 |
XG26H | 10.2-10.5 | -0,030 | 9.4-10.0 | ≥25 | -0.20 | 24-26 | 350 ℃ | 8.3 | |
XG28H | 10.3-10.8 | -0,035 | 9.5-10.2 | ≥25 | -0.20 | 26-28 | 350 ℃ | 8.3 | |
XG30H | 10.8-11.0 | -0,035 | 9.9-10.5 | ≥25 | -0.20 | 28-30 | 350 ℃ | 8.3 | |
XG32H | 11.0-11.3 | -0,035 | 10.2-10.8 | ≥25 | -0.20 | 29-32 | 350 ℃ | 8.3 | |
XG22 | 9.3-9.7 | -0,020 | 8.5-9.3 | ≥18 | -0.20 | 20-23 | 300 ℃ | 8.3 | |
XG24 | 9.5-10.2 | -0,025 | 8.7-9.6 | ≥18 | -0.20 | 22-24 | 300 ℃ | 8.3 | |
XG26 | 10.2-10.5 | -0,030 | 9.4-10.0 | ≥18 | -0.20 | 24-26 | 300 ℃ | 8.3 | |
XG28 | 10.3-10.8 | -0,035 | 9.5-10.2 | ≥18 | -0.20 | 26-28 | 300 ℃ | 8.3 | |
XG30 | 10.8-11.0 | -0,035 | 9.9-10.5 | ≥18 | -0.20 | 28-30 | 300 ℃ | 8.3 | |
XG32 | 11.0-11.3 | -0,035 | 10.2-10.8 | ≥18 | -0.20 | 29-32 | 300 ℃ | 8.3 | |
XG26M | 10.2-10.5 | -0,035 | 8.5-9.8 | 12-18 | -0.20 | 24-26 | 300 ℃ | 8.3 | |
XG28M | 10.3-10.8 | -0,035 | 8.5-10.0 | 12-18 | -0.20 | 26-28 | 300 ℃ | 8.3 | |
XG30M | 10.8-11.0 | -0,035 | 8.5-10.5 | 12-18 | -0.20 | 28-30 | 300 ℃ | 8.3 | |
XG32M | 11.0-11.3 | -0,035 | 8.5-10.7 | 12-18 | -0.20 | 29-32 | 300 ℃ | 8.3 | |
XG24L | 9.5-10.2 | -0,025 | 6.8-9.0 | 8-12 | -0.20 | 22-24 | 250 ℃ | 8.3 | |
XG26L | 10.2-10.5 | -0,035 | 6.8-9.4 | 8-12 | -0.20 | 24-26 | 250 ℃ | 8.3 | |
XG28L | 10.3-10.8 | -0,035 | 6.8-9.6 | 8-12 | -0.20 | 26-28 | 250 ℃ | 8.3 | |
XG30L | 10.8-11.5 | -0,035 | 6.8-10.0 | 8-12 | -0.20 | 28-30 | 250 ℃ | 8.3 | |
XG32L | 11.0-11.5 | -0,035 | 6.8-10.2 | 8-12 | -0.20 | 29-32 | 250 ℃ | 8.3 | |
Cathetan: · Kita tetep padha ing ndhuwur kajaba kasebut saka customer. Suhu Curie lan koefisien suhu mung kanggo referensi, ora minangka basis kanggo kaputusan.· Suhu kerja maksimum magnet bisa diganti amarga rasio dawa lan diameteripun lan faktor lingkungan. |
Kaluwihan:
Panganggone magnet iki dikondisikake kanthi suhu ing jarak sing amba saka 250ºC nganti 350ºC lan suhu Curie bisa dhuwur banget.
minangka 710 kanggo 880 ° C. Mulane, magnet SmCo duwe stabilitas Magnetik paling apik amarga resistance unggul kanggo suhu dhuwur.
SmCo wesi sembrani ditondoi dening resistance karat dhuwur banget, ora nutupi dibutuhake kanggo pangayoman lumahing.
Fitur:
Kerugian magnet SmCo yaiku brittleness sing ditandhani saka materi - faktor sing kudu digatekake sajrone proses.
Magnetik galvanis utawa dilapisi elektrodeposisi katodik kanggo aplikasi tartamtu.
Aplikasi:
Ing wilayah suhu operasi dhuwur, karat dhuwur lan resistance oksidasi sing wigati. Kayata, magnetron elektronik,Magnettransmisi ic,
Perawatan Magnetik, Magnistor, lsp.
Kabeh nilai kasebut ditemtokake nggunakake conto standar miturut IEC 60404-5. Spesifikasi ing ngisor iki dadi nilai referensi lan bisa uga
beda-beda. Maks. suhu operasi gumantung ing dimesion magnet lan aplikasi tartamtu. Kanggo informasi luwih lengkap hubungi kita
insinyur aplikasi.